Chemical Composition Limits | ||||||
Weight % | Cu | Ni | Mn | Fe | Pb | Zn |
NS 101 | 44-47 | 9-11 | 0.2-0.5 | 0.4 max | 1-2.5 | Remainder |
Nickel silvers can and have been used in industrial, rural and marine atmospheres but always needed an amount of maintenance work to keep them looking best. But now nickel silver has a new lacquer coating called “Incralac” which reduces the work needed.
Typical Mechanical PropertiesNS 101 | |
Ultimate Tensile Strength (N/mm²) | Elongation (%) |
460 | 8 |
Availability
NS101 is available in Bar, Rod, Sections, Sheet, Strip and Foil.
Specifications
BS 790: 1963: Sheet, Strip and Foil
BS 2874: 1986: Superceded by BS EN 12167, 12164 and 12163: 1998: Bar, Rod and Sections
Chemical Composition Limits | ||||||
Weight % | Cu | Fe | Mn | Ni | Pb | Zn |
NS 104 | 60-65 | 0.25 max | 0.05-0.30 | 11-13 | 0.4 max | Remainder |
Nickel silvers can and have been used in industrial, rural and marine atmospheres but always needed an amount of maintenance work to keep them looking best. But now nickel silver has a new lacquer coating called “Incralac” which reduces the maintenance work needed.
Typical Mechanical PropertiesNS 104 | |||||||
0.1% Proof Stress (Kg/mm²) | Tensile Strength (Kg/mm²) | Elongation (%) in 2" (50.8mm) | Vickers Hardness (HV) | ||||
A | E | A | E | A | E | A | E |
14.3 | 60.2 | 41 | 72 | 44 | 2 | 83 | 216 |
A - Annealed E-Extra Hard Cold Rolled |
Availability
NS104 is available in Sheet, Strip, Foil, Plate, Tube, Rod, Sections and Forgings.
Specifications
BS 1824: 1963: Strip and Foil
BS 2870: 1980: Superceded by BSEN1652, BSEN1653 and BSEN1654: Foil, Sheet and Strip
BS 2873: 1969: Superceded by BS EN12166: Wire
Chemical Composition Limits | ||||||
Weight % | Cu | Pb | Fe | Ni | Mn | Zn |
NS 106 | 60-65 | 0.03 max | 0.30 max | 17-19 | 0.05-0.50 | Remainder |
Nickel silvers can and have been used in industrial, marine and rural atmospheres but always needed an amount of maintenance work to keep them looking best. But now nickel silver has a new lacquer coating called “Incralac” which reduces the work needed.
Typical Mechanical PropertiesNS 106 | |||||||
0.1% Proof Stress (Kg/mm²) | Tensile Strength (Kg/mm²) | Elongation (%) in 2" (50.8mm) | Vickers Hardness (HV) | ||||
A | E | A | E | A | E | A | E |
44 | 72 | 20.3 | 59.8 | 39 | 2.2 | 93 | 216 |
A - Annealed E-Extra Hard Cold Rolled |
Availability
NS104 is available in Sheet.
Specifications
BS2870: 1980: Superceded by BSEN1652, BSEN1653 and BSEN1654: Foil, Sheet and Strip
BS2873: 1969: Superceded by BSEN12166: Wire
Chemical Composition Limits | ||||||
Weight % | Cu | Fe | Pb | Mn | Ni | Zn |
NS 752 UNS C75200 |
63-66.5 | 0.25 | 0.05 | 0.5 | 16.5-19.5 | Remainder |
Nickel Silver 752 is cold workable and has a high corrosion resistance.
Nickel Silver 752 (C75200) is available in Sheet, Plate, Bar, Rod, Strip, Wire. NS 752 Foil (Shim) is available in various thicknesses.